ISSN : 0970 - 020X, ONLINE ISSN : 2231-5039
     FacebookTwitterLinkedinMendeley

A New Method for Descaling Wool Fibres by Nano Abrasive Calcium Carbonate Particles in Ultrasonic Bath

Ali rezaghasemi 1, Safdar eskandarnejad1, Raminkhajavi2 and Mohammad Bameni Moghadam

1Textile Department Science and Research Branch Islamic Azad University, Tehran, Iran.

2Polymer and Textile Dept., South Tehran Branch, Islamic Azad University, Tehran, Iran.

3Department of Statistics, AllamehTabataba’I University, Tehran, Iran.

Corresponding Author E-mail: eskandarnejad@srbiau.ac.ir

DOI : http://dx.doi.org/10.13005/ojc/320456

Article Publishing History
Article Received on :
Article Accepted on :
Article Published : 06 Aug 2016
Article Metrics
ABSTRACT:

Up to now, the most conventional methods for descaling of wool fibre are based on chemical degradation and resin covering of scales or a combination of them. These methods are producing wastewater and can cover physical properties of the fibres beside scales orderly.  In this study, a new and clean method is developed on the basis of abrasion effect of calcium carbonate Nano particles (CCNP) in an ultrasonic bath. Woolen Samples (fibre and yarn) were sonicated with different levels of CCNP. Tensile properties of the yarns, directional friction effect of the fibres and scanning electron microscope images of the fibres were studied. Test results showed that sonicated Nano treatment of woolyarn reduced its tenacity, extension and work of rupture and increased its coefficient of friction. Scanning electron microscope images of fibres and measurement of fibres directional displacement confirmed descaling of Nano abrasive treated wool samples in comparison to the raw wool. 

KEYWORDS:

Wool; Descaling; Nano abrasive CaCO3; Ultrasonic; tenacity; directional friction; SEM

Download this article as: 

Copy the following to cite this article:

Alirezaghasemi, Safdareskandarnejad, Raminkhajavi, Moghadam M. B. A New Method for Descaling Wool Fibres by Nano Abrasive Calcium Carbonate Particles in Ultrasonic Bath. Orient J Chem 20016;32(4).


Copy the following to cite this URL:

Alirezaghasemi, Safdareskandarnejad, Raminkhajavi, Moghadam M. B. A New Method for Descaling Wool Fibres by Nano Abrasive Calcium Carbonate Particles in Ultrasonic Bath.Orient J Chem 20016;32(4). Available from: http://www.orientjchem.org/?p=20112


Introduction

Wool fibers form 3% of total world fibers consumed in the production of textiles [1]. Wool fabric shows a high amount of wrinkle resistance and stability of Shape which is due to the excellent recovery from deformations of the fibre. It possesses an outstanding thermal insulating power. This is partly due to the natural curliness of the fibre which causes a rather bulky cloth with much air in it. Wool is subject to biological attack; the fibre is readily eaten by moth larvae and some other insects, a fact which causes large economic losses. A second defect of wool is its shrinkage, this being an unwanted decrease of the dimensions of a fabric during its use [2].When a wool fabric is worked in presence of a solution of soap or acid, shrinkage takes place because the fibres migrate in the direction of their root ends, owing to the ratchet-like arrangement of the surface scales. During this migration a fibre which lies originally stretched in the yarn of which the fabric is composed, undergoes displacements and attains a looped and curled position [2].

The special feature of animal hair fibres by which they show felting power, is their scale structure which gives rise to a difference in friction in two directions along the fibre. Thus irreversible displacement occur, whereas for fibres without scales the total displacement under the influence of forces directed at random is Zero[2]. The friction of wool fibre depends on the direction in which it is pulled: the resistance is greater when it is pulled against the scales than when it is pulled with them. This is known as the directional frictional effect (D.F.E.) [3]. When a material containing wool fibres is submitted to mechanical action such as occurs in laundering or in fulling processes the fibres tend to migrate in the direction of their roots. This migration tendency is recognized as one of the principal factors in the formation of the entangled mass known as a felt, and in the excessive shrinkage which wool materials exhibit during laundering [4].

Martin showed that, D.F.E. still existed when a wool fibre was rubbed against a polished glass surface though no interlocking or ploughing action of the scales was to be expected in this case [5]. Rudall proposed a model with flexible scale tips; this model is also able to explain the decrease of D.F.E. after various chemical anti-shrink processes, in terms of softening or even a removal of the scale tips [6]. The first investigator who took notice of the influence of the scaliness on felting was Bowman. He introduced the interlocking scale theory in which the fibres are supposed to lock into each other by means of their scales and to form in this way an irreversible structure [7]. This theory met the criticism that the scale geometry is not regular enough to enable such interlocking over a number of consecutive scales and that microscopically this phenomenon is never observed. The theory was, therefore, modified in this respect that only few points of interlocking will occur on each fibre. Ditzel was the first who drew the attention to the role played by the root ends of the fibre [8].These ideas were taken up in 1944 by Martin who prepared some locks of wool by removing the scales from either the root ends or the tip ends [9].

Various attempts have been made to remove cuticle from wool by simple mechanical methods[10, 11, 12],by ultra-sonication [13]or simply shaking in formic acid [14, 15],or by more degradative chemical procedures [13]. Treatment in formic acid at room temperature causes very uneven removal of the cuticle [13].A treatment in boiling formic acid with agitation removes virtually all the cuticle from the fibres [13]. The optimum treatment for the removal of virtually all cuticle with minimal removal of cortical cells is a 20-min reflux in formic acid, followed by 16 hr. shaking in formic acid at room temperature [16].

Commercial methods of obtaining an unshrinkable finish on wool textile materials are based on chemical modification of the surface scale structure, although several methods are available for descaling fibres in the laboratory [17].King, for example, showed that single wool fibres can be descaled by drawing them under tension over the edge of a microscope slide [18], and human hair fibres was descaled by drawing between folded strips of emery paper under slight pressure [17].The use of enzymes to achieve wool shrink resistance, better whiteness and improved handle are also successfully employed in wool bleaching [19].In two hours the scale layers of the papain treated fibres were completely destroyed and resulted in a smooth surface without any scales. For longer periods (more than two hours) the effects of the trypsin attacks on the scales are presented elsewhere [20].

Chlorination process causes damages to cuticle layer of wool and hence deterioration of strength and work of rupture in general [21]. Wool scoured in ultrasonic bath has less fibre felting. Coefficient of friction of fabrics treated in ultrasound bath increased due to a change in texture of surface fibres [21]. An increase in intensity of ultrasonic waves during washing process could reduce fabric strength, although Li et al. showed that washing in ultrasonic bath didn’t change fabric strength significantly [22,23]. Surface of wool fibre is greasy and polluted, and must be washed at a stage. It is reported that, chemistry of the effluent generated by scouring of fine quality Merino wool was different from that of Indian carpet grade wool [24]. Corona discharge is being used widely to modify surface texture of textiles and polymers. It is reported that, an increase in power and number of corona treatments increased cracks and hoes on the surface of the treated leather [25]. Wool fabrics can be made unshrinkable by impregnating them with oil and a finely divided abrasive, followed by mechanical working in a milling machine. Under these conditions the scale edges of the fibres are removed and effectiveness of the abrasive increases with increasing fineness and hardness. Among a large number of powders examined, 200-mesh (I.M.M.) silica gave the highest degree of unshrinking ability [17].

The purpose of this research for descaling of wool is to avoid chemical methods and use mechanical ones together with application of a Nano abrasive material with suitable hardness. If this process is successful, it could be an eco-friendly method of wool descaling and prevent environmental pollution.

Experimental

Materials

Raw material used was 23Tex wool/polyester (45-55) single yarn and raw woolfibre with mean diameter of 35 Micron. The abrasive material used was calcium carbonate Nano particle (60 nm) and chemicals of sodium hypochlorite (NaOCl) and hydrochloric acid (HCl).

Methods

Yarn samples were immersed loosely in an ultrasonic bath of 35 KHz, 40 watt, containing calcium carbonate Nano particles (CCNP) in different concentrations of 2, 6 and 10g/lit.The yarns were descaled at 37ﹾC temperature for 35min. In order to prevent twist loss of the yarns, both ends of the yarn samples were tied together. Usually results of a new experiment must be compared with an ordinary one. In this study, results were compared with chlorination method of descaling as an ordinary one. One of the samples were chlorinated in ultrasonic bath in order to recognize effect of sonication on chlorination method of descaling. The yarns were coded as R for raw wool, U for ultrasound treated, C for chlorinated, N for Nano treated together with 2, 6 and 10 for concentrations of 2, 6 and 10 g/lit. Table 1 shows yarn treatment codes for fibre and yarn.

Table 1: Fibre andyarn codes 

Treatment

Code

Sample

Raw wool

R

1

Sonicated raw wool

U

2

Sonicated in 2 g/lit Nano material

UN2

3

Sonicated in 6 g/lit Nano material

UN6

4

Sonicated in 10 g/lit Nano material

UN10

5

Chlorinated

C

6

Chlorinated in ultrasonic bath

CU

7

 

Mechanical properties such as strength, elongation and work of rupture of the yarns were measured on anElima tensile tester which works on the base of constant rate of elongation (CRE). A gauge length of 25 cm, clamp speed of 20 cm/min were used and 20 samples were tested in each case.

To determine the coefficient of friction of yarns, four glass rods with a diameter of 17 mm assembled on the yarn tensile tester (as shown in Figure 1).Yarn samples were threaded as shown in Fig.1 to the moving clamp (A) and a 5 g weigh of D. The pulling force with a contact angle of 720° at the clamp speed of 25 cm/min was measured.

Figure 1.Schematic diagram of yarn path for determination of yarn coefficient of friction Figure 1: Schematic diagram of yarn path for determination of yarn coefficient of friction
Click here to View Figure

 

Displacement of fibre towards the root was used as a measure of descaling. If a wool fibre is rubbed along its length in a reciprocal mode, quality and form of its scales will determine its displacement toward the root. The lower the displacement, the higher is the damage to the scales. This principle was used for evaluation of descaling. For this purpose, the fibres were rubbed reciprocally along their length for an amplitude of 20mm between two glass plates of A and B. The button glass (A) was covered with amm-scaled paper and the upper glass (B) was first covered with a sponge layer of 1.5 mm thickness and then with a layer of 80 g/m2 paper. Each fibre was rubbed for 10 cycles and the displacement was recorded. Ten fibres were tested in each case. The test parameters were selected by trial and error and according to the results of a M.Sc. dissertation [26]. Figure 2 shows schematic diagram of the plates and the fibre. For studying surface of the fibres, LEO Scanning Electron Microscope model 440i (SEM) was used. The fibres were coated with gold prior to SEM imaging.

 

Figure 2.Glass plates for measurement of directional displacement [26]  A- Flat glass covered by mm-scaled paper B- Flat glass covered by sponge and a sheet of paper C- Wool fibre located between two glass plates

Figure 2: Glass plates for measurement of directional displacement [26]

A- Flat glass covered by mm-scaled paper

B- Flat glass covered by sponge and a sheet of paper

C- Wool fibre located between two glass plates



Click here to View Figure

Results and Discussion

Test results of yarn tenacity, strain at peak, work of rupture and coefficient of friction are given in figure 3. Analysis of variance of yarn properties (ANOVA) for comparison of means and Tukey test for ranking of yarn properties are given in tables 2 and 3.

 

Figure 3: Results of yarn properties  A- Yarn tenacity (cN/tex)    B- strain at beak (%)  C- Work of rupture               D- Coefficient of friction

Figure 3: Results of yarn properties

A- Yarn tenacity (cN/tex)    B- strain at beak (%)

C- Work of rupture               D- Coefficient of friction

 

Click here to View Figure

 

Table 2: Analysis of variance (ANOVA) of yarn properties

Sum of Squares

df

Mean Square

F

Sig.

Tenacity(cN/tex) Between Groups

36.914

6

6.152

2.139

0.05

Within Groups

382.603

133

2.877

Total

419.518

139

Strain at peak Between Groups

971.577

6

161.929

42.649

0.00

Within Groups

504.979

133

3.797

Total

1476.556

139

Work of Rupture Between Groups

2.742

6

.457

4.024

0.00

Within Groups

15.106

133

.114

Total

17.848

139

Friction Between Groups

.001

6

.000

3.436

0.00

Within Groups

.002

63

.000

Total

.002

69

 

Table 3: Tukey test of ranking for results of yarn properties

Table 3: Tukey test of ranking for results of yarn properties

Table 3: Tukey test of ranking for results of yarn properties



Click here to View table

 

According to ANOVA test for yarn properties in table 2, sig. values of 0.05, 0.00, 0.00 and 0.00, indicate that there are a significant statistical difference between the means of yarn properties. Strength of yarns UN10 and R were minimum (12.4 cN/tex) and maximum (14.0 cN/tex) respectively. There was no significant difference between tenacity of rest of the yarns with UN10 and R yarns. Concentration of the Nano abrasive in the rage of 2 to 10 g/lit didn’t affect yarn tenacity.

Results of yarn strain in table 3 shows that, strain of UN10 and UN2 yarns were significantly lower than that of R yarn. There was no difference between strains of the above yarns with rest of the yarns. Therefore, concentration of nano-CaCO3 didn’t have significant effect on strain of the yarns. Also, sonication affected yarn strain in comparison to the raw wool, but it didn’t hasany effect on chlorinated yarn. Behavior of work of rupture of the yarns were the same as their strain. Tukey test of ranking for yarn coefficient of friction (YCF) in table 3 shows that, YCF of UN10 is significantly greater than that of R, U and UN2 yarns. There is no difference between YCF of the above mentioned yarns with rest of the yarns. Therefore, sonication didn’t have any effect on YCF of the raw wool and the increase in concentration of Nano abrasive material from 2 to 10 g/lit increased YCF significantly.

Directional frictional effect (DFE) of the fibres was evaluated with directional displacement of the fibres (DDF) due to a reciprocal rubbing action between two glass plates as described in 2.2. Results of DDF are given in figure 4. ANOVA of DDF results and their Tukey test of ranking are given in tables 4 and 5. Significance value of the ANOVA of DDF in table 4 is 0.00 and indicates that there is a difference between the means. Tukey test of ranking shows that, DDF of R and U fibres are significantly greater than that of rest of the fibres. It may be concluded that, chlorination and Nano treatment of the fibres affect their DFE to the same extent and concentration of the Nano particle in the range of 2 to 10 g/lit doesn’t have any effect on DFE of the fibres.

Figure 4: Mean directional displacement of fibres

Figure 4: Mean directional displacement of fibres



Click here to View Figure

 

Table 4: Analysis of variance (ANOVA) of directional displacement of fibres

Sum of Squares

Df

Mean Square

F

Sig.

Between Groups

6267.143

6

1044.524

9.986

0.00

Within Groups

6590.000

63

104.603

Total

12857.143

69

 

Table 5: Tukey test of ranking for directional displacement of fibres

  code

N

Subset for alpha = 0.05

1

2

TukeyHSDa CU

10

18.00

UN10

10

20.50

UN2

10

21.00

UN6

10

21.50

C

10

21.50

U

10

40.00

R

10

42.50

Sig.

0.98

0.99

 

To investigate effect of Nano abrasive on surface of the fiber, scanning electron microscope (SEM) images of surface of the fibres were studied.Figure 5 shows SEM images of the fibres. A comparison of raw and sonicated wool in R and U samples doesn’t show a clear difference in terms of scale removal. But, effect of the increase in concentration of CCNP from 2 to 10 g/lit is obvious and may be observed in UN2, UN6 and UN10 samples. Sharpness of edge of the scales start to worn in UN2 fibre, it intensifies in UN6 and finally becomes nearly flat in UN10 fibre. This indicates that, sonicated Nano abrasive treatment modifies surface of the fibre effectively and it intensifies with the increase in concentration of the CCNP. Edge of the scales are worn and lost their sharpness in chlorinated and ultrasound assisted chlorinated samples C and CU.  It is difficult to recognize effect of sonication on chlorinated wool when there is a reasonable wear of the scales.

Scales lost their sharpness in descaling and it reduced directional coefficient of friction of the fibre. As a result directional displacement of the fibre reduced, which causes wool felting.

Figure 5: SEM images of samples

Figure 5: SEM images of samples

 

Click here to View Figure

 

Conclusions

It may be concluded from the test results that, Nano abrasive treatment removed a thin layer from surface of the fibres and changed sharpness of the scales. Tenacity, strain and work of rupture of the Nano abraded sample (UN10) reduced and its coefficient of friction increased in comparison to the raw wool, which is not avoidable in other methods of descaling as well. Directional displacement of the fibre, as a measure of directional friction and felting intensity, decreased for Nano treated and chlorinated samples. SEM images showed that, scales could be modified (UN6) or nearly removed (UN10) with this method. Since the Nano abraded material is recyclable and this method of descaling doesn’t have any pollutant for our environment, it may be used as a novel, green and environmental friendly method of wool descaling instead of other commercial and environmentally pollutant methods.

References

  1. Zahn, H.; Wool, Aachen,Federal Republic of Germany.2005, 1
  2. Van Der Vegt, A.K.; A Study on the Mechanism of Wool Felting, UitgeverijExcelsior.1996, 957-963
  3.  Morton, W.E., Hearle, J.W.S.; Physical Properties of Textile Fibers.Textile Institute. 1993,635.
  4. Frishman, D., Smith, A. and Harris, M.; Measurement of the Frictional Properties of Wool Fibers. Textile Research Journal.1948, 475-480.
    CrossRef
  5. Martin, A.J.P.In ‘Van Der Vegt, A.K.; A Study on the Mechanism of Wool Felting, UitgeverijExcelsior.1996, 957-963’.
  6. Rudall, K.M. in ‘Van Der Vegt, A.K.; A Study on the Mechanism of Wool Felting, UitgeverijExcelsior.1996, 957-963’.
  7. Bowman, F.H., in ‘Van Der Vegt, A.K.; A Study on the Mechanism of Wool Felting, UitgeverijExcelsior.1996, 957-963’.
  8. Ditzel, W., In ‘] Van Der Vegt, A.K.; A Study on the Mechanism of Wool Felting, UitgeverijExcelsior.1996, 957-963’.
  9. Martin, A.J.P. (1944), In ‘] Van Der Vegt, A.K.; A Study on the Mechanism of Wool Felting, UitgeverijExcelsior.1996, 957-963’.
  10. Bradbury, J.H.; Separation and analysis of scale-Rich Material from Wool. Nature.1959,183,305-306.
    CrossRef
  11. Haly, A.R.; the Propagation of Excitation Energy in Keratin. Trans. Far. Soc.1960, 56, 1252-1259.
    CrossRef
  12. Snaith, J.W.; A Method of Removing the Outer Layers of Animal Fibers.Textile Research Journal.1960, 30,543.
    CrossRef
  13. Bradbury, J.H. and Chapman, G.V.; The Chemical Composition of Wool,part1: The Separation and Microscopic characterization of Components Produced by Ultrasonic Disintegration, Aust. J. Biol. Sci.1964,17, 960- 972.
    CrossRef
  14. Bradbury, J.H. and Chapman, G.V. and King, N.L.R.;The Chemical Composition of Wool,part3: Analysis of Cuticle, Skin Flakes and Cell Membrane Material, Proc. Third Intern. Wool Textile Res. Conf., Paris. 1965, 359- 366.
  15. Bradbury, J.H., chapman, G.V. and King N.L.R.; Separation of ChemicallyUnmodified Histological Components of Keratin Fibers and Analysis of Cuticles, Nature.1966, 210, 1333-1334.
    CrossRef
  16. Bradbury, J.H. and Peters, D.E.; Method for the Complete Removal of Cuticle from Wool Fibers, Textile Research Journal. 1972, 42:4, 248-250.
    CrossRef
  17. Speakman, J.B. and Whewell, E.; the Use of Abrasives to Make Wool Unshrinkable, Journal of the Textile Institute Transaction. 1945,36:3, 48-56.
    CrossRef
  18. King, in‘Speakman, J.B. and Whewell, E.; the Use of Abrasives to Make Wool Unshrinkable, Journal of the Textile Institute Transaction. 1945,36:3, 48-56.’
    CrossRef
  19. Schumacher, K. and Heine E.; Extremozymes for Improving Wool Properties. J. Biotechnology. 2001, 89, 281-288.
    CrossRef
  20. Goudarzi, G., Sepehrizadeh, Z., TabatabaeiYazdi,M. and Jamshidiha,M.; Comparison of Surface Modification of WoolFibres Using Pronase, Trypsin, Papain and pepsin. Fibres& Textiles in Eastern Europe.2008,90-92
  21. Khajavi, R. and Azari, P.; Effect of Ultrasound Irradiation on Wet WoolChlorination Treatment. Pakistan Journal of Biological Sciences.2007, 10, 2732-2735.
    CrossRef
  22. Li, Q., Lin, T., Wang,X.; Effects of Ultrasonic Treatment on Wool Fibre and Fabric Properties. J.Text. Inst. 2012, 103 (6), 662-668.
    CrossRef
  23. Li, Q., Hurren, C.J., Yu, H., Ding, C., Wang, X. Thermal and Mechanical Properties of Ultrasonically Treated Wool. Text. Res. J. 2012. 82 (2), 195-202.
    CrossRef
  24. Daga K, Loonker S, Gupta V, Singh A. V, Rajendra. Physico-Chemical Investigation on Carpet Grade Wool and its Effluent.Orient J Chem2001;17(3).
  25. Maleknia L, Fard G. C, Ekhlasi F. Study effect corona discharge on morphology, wettability and antibacterial of leather. Orient J Chem2015;31(Special Issue1).
  26. Ghavidel H.; M.Sc. Dissertation, Science and Research Branch Islamic Azad University, Tehran, Iran.2009.


Creative Commons License